牌号 400
对应标准 AS /NZS 3678-2016
热轧结构钢板、波纹板和厚板
Structural steel - Hot-rolled plates, floorplates and slabs
归类 合金钢
400 化学元素成分含量(%)
成分 C Si Mn P S Cr Ni Cu Mo Ti V Nb Al 更多
最小值 - - - - - - - - - - - - - Nb+V+Ti≤0.15;Cr+Ni+Cu+Mo≤1;Ceq≤0.48
最大值 0.22 0.55 1.7 0.04 0.03 0.25 0.3 0.4 0.35 0.04 0.1 0.06 0.1
①The use of sulfide modification steelmaking techniques (such as Ca addition) is permitted for listed grades
②For Z25 grades sulfur 0. 008% maximllm. Z35 grades sulfur 0.005% maximum.
③Boron shall not be int entionally added to the steel without the agreement of the purchaser
400 机械性能
条件 热处理或状态
抗拉强度
σb
Mpa
屈服点
σs
Mpa
断后伸长率或延伸率
δ
%
板材和底板(地板用花纹板);t≤12 热轧 ≥480 ≥400 ≥18
板材和底板(地板用花纹板);12<t≤20 热轧 ≥480 ≥380 ≥18
板材和底板(地板用花纹板);20<t≤80 热轧 ≥480 ≥360 ≥18
板材和底板(地板用花纹板);80<t≤150 热轧 ≥480 ≥18
板材和底板(地板用花纹板);150<t≤200 热轧 ≥17
①For test piece cross-sectional area > 1000 mm<sup>2</sup>, minimum elongation is reduced by 2%
②Suffix Z added to grade designation indicates that material has been through-thickness tested. Minimum reduction of area: 15% for grade suffix Z15, 25% for grade suffix Z25 and 35% for grade suffix Z35.

材料牌号对应供应商

告诉我在“材数库”看到,将给您优惠

1
主营: 压力容器用钢板 低合金度钢板 耐磨钢板 耐腐蚀钢板 合金结构钢板 碳素结构钢板 模具用钢板 桥梁用钢板 高层建筑结构用钢板
  • 联系人:刘经理
  • 移动电话: 18236617771
  • 电话:13603751926
  • 微信号:TEL13603751926
板材6mm-100mm热轧
400 对应不同标准
1 AS /NZS 3678-2016 热轧结构钢板、波纹板和厚板
400
2 AS /NZS 3679-1-1996 第 1 部分: 热轧钢筋和型钢
400
注:数据仅供参考!如有疑问,请填写"我要纠错"!
版权说明:
⑴ 本网站的所有内容(包括但不限于文字、图片、音频、视频等)均受到版权保护,版权归本网站所有;
⑵ 未经授权,禁止以任何形式转载、复制、传播或用于其他商业用途;
⑶ 如需使用本网站内容,请提前获得授权。